Surface free energy of solids

We have put together a list of frequently used solids and their surface free energies for you from our literature database. This list is only a selection of important substances with the surface free energy as a basic value. Don't hesitate to contact us for more detailed information about the substances as well as the literature sources:

  • partition of the surface free energy into a disperse and a polar fraction
  • further partition of the polar fraction into an acid and a base component
  • fraction of hydrogen bridge bonds (Extended FOWKES method)
  • related temperature for the data

Values for the surface free energy (SFE) of solids 

Substance

SFE
(mN/m)     

CAS
number

ABS

41.90

n.a.

acyclovir

47.80

59277-89-3

acyclovir

51.20

59277-89-3

alumina (aluminium-oxide Al2O3)

31.00 

1344-28-1

alumina (aluminium-oxide AI2O3)

38.66

1344-28-1

alumina (aluminium-oxide AI2O3)

40.09

1344-28-1

alumina (aluminium-oxide AI2O3)

48.19

1344-28-1

alumina (aluminium-oxide AI2O3)

50.50

1344-28-1

aluminium

33.00

7429-90-5

aluminium

35.00

7429-90-5

bariumsulfate (barytes) BaSO4

26.70

7727-43-7

bariumsulfate (barytes) BaSO4

43.40

7727-43-7

beta-copperphthalocyanin

33.00

147-14-8

calciumcarbonate CaCO3

25.10

471-34-1

calciumcarbonate CaCO3

33.10

471-34-1

carbon

34.80

7440-44-0

carbon-black

37.00

133-86-4

carbon-black

40.00

133-86-4

chromium-nitride (CrN)

38.00

12053-27-9

clay

31.30

1318-74-7

clay

45.67

1318-74-7

clay

51.71

1318-74-7

clay

55.50

1318-74-7

clay

60.60

1318-74-7

clay

60.70

1318-74-7

clay

62.00

1318-74-7

clay

65.80

1318-74-7

clay

66.00

1318-74-7

FEP (flourinated ethylene propylene copolymer)

18.70

25067-11-2

FEP (flourinated ethylene propylene copolymer)

19.00

25067-11-2

germanium

55.00

7440-56-4

glass

43.10

n.a.

glass

65.00

n.a.

glass

66.50

n.a.

glass

68.00

n.a.

glass

69.50

n.a.

glass

70.30

n.a.

glass

73.00

n.a.

glass

73.30

n.a.

glass

112.90

n.a.

hafnium-carbide (HfC)

36.00

11129-37-6

hafnium-carbide (HfC)

39.00

11129-37-6

hafnium-nitride (HfN)

39.00

25817-87-2

hexatriacontan

21.00

630-06-8

HPMC (hydroxypropylmethylcellulose)

41.60

9004-65-3

HPMC (hydroxypropylmethylcellulose)

45.70

9004-65-3

HPMC (hydroxypropylmethylcellulose)

58.40

9004-65-3

iron-oxide

28.00

1309-37-1

iron-oxide

32.90

1309-37-1

lactose

55.30

5965-66-2

lactose

57.20

5965-66-2

lactose

69.40

5965-66-2

magnesium oxide

46.98

1309-48-4

magnesium oxide

46.99

1309-48-4

magnesium oxide

47.01

1309-48-4

magnesium oxide

47.04

1309-48-4

mica

36.10

12001-26-2

mica

45.70

12001-26-2

mica

67.10

12001-26-2

mica

120.00

12001-26-2

monoazo-red

47.00

5280-66-0

monoazo-yellow

37.00

6528-34-3

n-hexatriacontane

18.74

762-42-5

n-octadecyl-amine

23.01

124-30-1

NR (natural rubber)

18.00

9003-31-0

omega-monohydro-perflouro-undecanoic-acid

18.73

1765-48-6

PA 6 (polycaprolactam)

38.00

25038-54-4

paraffin

19.00

8002-74-2

paraffin

23.66

8002-74-2

paraffin

25.09

8002-74-2

paraffin

25.10

8002-74-2

paraffin

25.50

8002-74-2

PBT (polybutylene terephthalate)

45.00

25971-63-5

PC (polycarbonate)

29.00

25971-63-5

PC (polycarbonate)

32.60

25971-63-5

PC (polycarbonate)

38.80

25971-63-5

PDMS (polydimethylsiloxane)

22.10

63148-62-9

PE (polyethylene)

27.00

9002-88-4

PE (polyethylene)

31.80

9002-88-4

PE (polyethylene)

32.10

9002-88-4

PE (polyethylene)

32.39

9002-88-4

PE (polyethylene)

32.82

9002-88-4

PE (polyethylene)

33.00

9002-88-4

PE (polyethylene)

33.10

9002-88-4

PE (polyethylene)

33.20

9002-88-4

PE (polyethylene)

35.00

9002-88-4

PE (polyethylene)

35.10

9002-88-4

PE (polyethylene)

36.00

9002-88-4

PE (polyethylene)

36.30

9002-88-4

pentoxyfilline

56.20

6.5.6493

pentoxyfilline

68.50

6.5.6493

pentoxyfilline

77.10

6.5.6493

PET (polyethyleneterephthalat)

37.40

25038-59-9

PET (polyethyleneterephthalat)

39.48

25038-59-9

PET (polyethyleneterephthalat)

39.50

25038-59-9

PET (polyethyleneterephthalat)

40.90

25038-59-9

PET (polyethyleneterephthalat)

41.30

25038-59-9

PET (polyethyleneterephthalat)

42.20

25038-59-9

PET (polyethyleneterephthalat)

42.35

25038-59-9

PET (polyethyleneterephthalat)

44.00

25038-59-9

PET (polyethyleneterephthalat)

46.50

25938-59-9

PMMA (polyethylmethacrylate)

38.70

9003-42-3

PMMA (polyethylmethacrylate)

39.00

9003-42-3

PMMA (polyethylmethacrylate)

39.70

9003-42-3

PMMA (polyethylmethacrylate)

41.20

9003-42-3

PMMA (polyethylmethycrylate)

41.40

9003-42-3

PMMA (polyethylmethacrylate)

43.80

9003-42-3

PMMA (polyethylmethycrylate)

44.60

9003-42-3

PMMA (polyethylmethacrylate)

44.90

9003-42-3

PMMA (polyethylmethacrylate)

45.80

9003-42-3

polychloroprene

43.50

9010-98-4

polychlorotrifluoroethylene

26.93

9002-83-9

polychlorotrifluoroethylene

29.80

9002-83-9

polychlorotrifluoroethylene

31.00

9002-83-9

polyvinylidene-chloride

40.00

9002-85-1

polyvinylidene-chloride

41.34

9002-85-1

PP (polypropylene)

28.00

9003-07-0

PP (polypropylene)

29.40

9003-07-0

PP (polypropylene)

29.70

9003-07-0

PP (polypropylee)

30.70

9003-07-0

PP (polypropylene)

31.20

9003-07-0

PP (polypropylen)

31.80

9003-07-0

PP (polypropylene)

32.10

9003-07-0

PP (polypropylene)

34.10

9003-07-0

PS (polystyrene)

29.20

9003-53-6

PS (polystyrene)

38.00

9003-53-6

PS (polystyrene)

39.00

9003-53-6

PS (polystyrene)

40.57

9003-53-6

PS (polystyrene)

40.80

9003-53-6

PS (polystyrene)

41.90

9003-53-6

PS (polystyrene)

42.00

9003-53-6

PS (polystyrene)

42.80

9003-53-6

PTFCE (polytrifluorochloroethylene)

28.30

9002-83-9

PTFE (polytetrafluoroethylene)

15.56

9002-84-0

PTFE (polytetrafluoroethylene)

16.60

9002-84-0

PTFE (polytetrafluoroethylene)

18.50

9002-84-0

PTFE (polytetrafluoroethylene)

19.00

9002-84-0

PTFE (polytetrafluoroethylene)

19.10

9002-84-0

PTFE (polytetrafluoroethylene)

20.00

9002-84-0

PTFE (polytetrafluoroethylene)

20.70

9002-84-0

PTFE (polytetrafluoroethylene)

21.77

9002-84-0

PVA (polyvinylalcohol)

37.00

9002-89-5

PVA (polyvinylalcohol)

38.80

9002-89-5

PVAc (polyvinylacetate)

36.50

9003-20-7

PVAc (polyvinylacetate)

41.00

9003-20-7

PVC (polyvinylchloride)

27.00

9002-86-2

PVC (polyvinylchloride)

33.00

9002-86-2

PVC (polyvinylchloride)

33.10

9002-86-2

PVC (polyvinylchloride)

36.70

9002-86-2

PVC (polyvinylchloride)

38.10

9002-86-2

PVC (polyvinylchloride)

39.50

9002-86-2

PVC (polyvinylchloride)

39.62

9002-86-2

PVC (polyvinylchloride)

40.00

9002-86-2

PVC (polyvinylchloride)

41.50

9002-86-2

PVC (polyvinylchloride)

42.90

9002-86-2

PVC (polyvinylchloride)

44.10

9002-86-2

PVDF (polyvinylidenefluoride)

25.00

24937-79-9

PVDF (polyvinylidenefluoride)

32.10

24937-79-9

PVDF (polyvinylidenefluoride)

32.28

24937-79-9

PVDF (polyvinylidenefluoride)

32.70

24937-79-9

PVP (polyvinylpyrrolidone)

44.30

9003-39-8

PVP (polyvinylpyrrolidone)

44.60

9003-39-8

PVP (polyvinylpyrrolidone)

50.40

9003-39-8

stearic acid

21.80

57-11-4

steel

29.00

7439-89-6

steel

34.40

7439-89-6

steel

35.00

7439-89-6

steel

43.00

7439-89-6

steel

43.80

7439-89-6

steel

44.50

7439-89-6

steel

45.00

7439-89-6

steel

46.30

7439-89-6

steel

50.50

7439-89-6

steel

53.90

7439-89-6

steel

56.00

7439-89-6

talc

42.90

14807-96-6

talc

48.00

14807-96-6

tin

41.00

7440-31-5

tin

67.40

7440-31-5

titanium

46.50

7440-32-6

titanium-dioxide

27.70

13463-67-7

titanium-dioxide

35.60

13463-67-7

titanium-dioxide

35.90

13463-67-7

titanium-dioxide

39.90

13463-67-7

titanium-dioxide

40.70

13463-67-7

titanium-dioxide

41.10

13463-67-7

titanium-dioxide

42.90

13463-67-7

titanium-nitride (TiN)

43.00

25583-20-4

tungsten-carbide (WC)

46.30

12070-12-1

zircona (zirconium-oxide ZrO2)

42.04

1314-23-4

zircona (zirconium-oxide ZrO2)

42.54

1314-23-4

zircona (zirconium-oxide ZrO2)

42.61

1314-23-4

zircona (zirconium-oxide ZrO2)

42.75

1314-23-4

zirconium-carbide (ZrC)

35.00

12070-14-3

zirconium-carbide (ZrC)

37.00

12070-14-3

zirconium-nitride (ZrN)

40.00

25658-42-8

 

 

 